Re: Soldering to Paladium vs. Tin_Lead plated comps

Electronics Forum | Fri Feb 20 09:41:11 EST 1998 | Chrys Shea

| I have been involved in SMT for only a few months so I am coming from a position of extreame ignorance. I have been asked to investigate the differences in soldering to components with Paladium coated leads vs the standard Tin_lead. I would appre

Re: white dirty solder

Electronics Forum | Mon Jan 26 11:46:16 EST 1998 | Rin Or

| I have a problem! The solder on my pc boards look great comeing out | of my reflow oven. They go thrue the rest of the prossese | and at the end at the qc station it's cold or whitish or gray not shiny. | does any one have a idea on how to correct

Re: white dirty solder

Electronics Forum | Mon Jan 19 20:25:52 EST 1998 | Steve Gregory

| I have a problem! The solder on my pc boards look great comeing out | of my reflow oven. They go thrue the rest of the prossese | and at the end at the qc station it's cold or whitish or gray not shiny. | does any one have a idea on how to correct

Specification for Screw Torques

Electronics Forum | Tue Nov 06 18:39:08 EST 2001 | MikeF

Also, check the website for Assembly magazine, http://www.assemblymag.com, they have some good information on the basics of torque. Determining the "correct" torque value can become very complicated very quickly. The same size screws made from differ

Lead laws threaten electronics

Electronics Forum | Wed Nov 07 11:27:28 EST 2007 | patrickbruneel

Grant, Thanks for sharing that experience with us; this comes to show what damage can be done when politicians make laws based on rumors instead of facts. New laws as drastic as removing lead in soft soldering should have been based on scientific e

Tracking labor at selective solder

Electronics Forum | Thu Dec 21 15:13:16 EST 2017 | georgetruitt

Is the process the same for every product running through the selective solder machine? Load program, acquire or set up fixture, Change/load flux?, Change/Load solder pot? Are the machines cold when the operators need to use them or are the machin

Re: Suspect BGAs

Electronics Forum | Wed Mar 17 02:14:39 EST 1999 | Joe

| | We are having a small number (~2%) of our boards pass our manufacturing diagnostics, fail once they reach the customer, fail when they get back to us and then start working again after handling them for a short time. We have eliminated a lot of

Flason SMT Products

Electronics Forum | Wed Oct 03 23:58:23 EDT 2018 | gaintstar

Flason SMT News: http://www.flason-smt.com/new/6-Things-to-Check-Before-Submitting-Your-PCB-Design-for-Manufacturing.html http://www.flason-smt.com/new/about-wave-soldering-machine-tin-pot.html http://www.flason-smt.com/new/Advantages-of-Design-for-


cold solder-joint searches for Companies, Equipment, Machines, Suppliers & Information

Sell Your Used SMT & Test Equipment

Easily dispense fine pitch components with ±25µm positioning accuracy.
Selective soldering solutions with Jade soldering machine

Wave Soldering 101 Training Course
Equipment Auction Automotive Electronics Supplier - Closure of Tier-One SMT Dvision: (10) ASM & Universal SMT Lines & Feeders Equipment as-new-as 2019! Dek | Koh Young | Speedline | Vitronics | Viscom

Best Reflow Oven
2024 Eptac IPC Certification Training Schedule

World's Best Reflow Oven Customizable for Unique Applications