Electronics Forum | Thu Sep 02 07:50:27 EDT 2010 | sachu_70
Just to add to my comments,solder joint voids do occur in LGA. Voids in LGA can be larger due to geometry and greater ratio of flux to solder. IPC-A-610D specifies a greater than 25% voided area is a defect for BGA, however, it does not specify the d
Electronics Forum | Thu Sep 09 05:23:10 EDT 2010 | 15009
You can reduce and almost eliminate voids and other paste related defects in LGA's BGA's, QFN's etc, by using solid solder deposit. Its been around for 24 years, 13 in the US. It is now included in the new IPC 7093 specification for bottom terminat
Electronics Forum | Tue Jul 26 08:20:46 EDT 2005 | Bob R.
All you can do is try it. I did a literature search last year on causes of BGA voiding and came up with a pretty long list, sometimes contradictory. I also discussed it with several paste suppliers. What I came away with is that what aggravates voi
Electronics Forum | Tue Jul 02 02:50:55 EDT 2002 | ianchan
Hi mates, was going thru the IPC-A-610C Standards, and noted BGA voids stands somewhere between 10%-25% voids permissible in the solder "ball" bump, after reflow process. Was wondering, hypothetical case study, is there any specification for voids
Electronics Forum | Tue Mar 09 17:52:05 EST 2004 | davef
Bryan: Comments are: * You're correct, solder paste formualtion is a major driver to voiding in BGA balls. * Voids are primarily process indicators. There is experimental evidence that voids retard crack propagation locally around the void on a temp
Electronics Forum | Thu Oct 26 18:10:11 EDT 2000 | ptvianc
Philip: Cases 1-3, those criteria may be specified in more recent versions of ANSI/J-STD-001 and/or ANSI/IPC-A-610. Unfortunately, I do not have any new versions of these specs. that may cover these points. As for voids in BGA joints, I have not
Electronics Forum | Sun Aug 10 21:57:25 EDT 2014 | cmchoue
Does IPC definition for "QFN Void Ration" ? Like IPC 7095 susgestion the BGA Void ratio.
Electronics Forum | Sat Mar 06 02:54:25 EST 2004 | tommy
1)Solder paste selection 2)Reflow profile.Focus on soaking and TAL. 3)Moisture control for BGA. 4)Maybe the BGA solder ball already with void. 5)PCB design.Any via on bga land? 6)Solder masking type. 7)Solder paste volume apply on land. 8)IPC class 3
Electronics Forum | Tue Nov 26 09:07:16 EST 2019 | scotceltic
I am more worried about those voids also instead of the voids in the thermal pads. I still can't find any IPC spec that calls out a min. void percentage other than on BGA packages.
Electronics Forum | Mon Mar 27 20:59:41 EST 2000 | Dave F
Garo: Voids are primarily process indicators. There is experimental evidence that voids retard crack propagation locally around the void on a temporary basis. There is no standard, IPC or otherwise, on voids--nor should there be. See also J-STD-013,
IPC is the trade association for the printed wiring board and electronics assembly industries.
Training Provider / Events Organizer / Association / Non-Profit
3000 Lakeside Drive, 309 S
Bannockburn, IL USA
Phone: 847-615-7100