Electronics Forum | Mon Sep 20 11:21:48 EDT 2010 | tony1
I have this NiPdAu small QFN packge sizes less than 2x2. I tried to do solderability Dip And Look test and there's always some units no wet on either ground pad and small I/O. Can someone help to explain why is this so difficult to set on this surfac
Electronics Forum | Wed Sep 22 15:33:54 EDT 2010 | davef
Comments are: * First, no one is looking at your posting. You need to post in the 'SMTnet Production Forum' [top of the page]. This 'SMTnet Site Support Forum' is for whiners that want to complain to Neil about problems in logging-in, font that's to
Electronics Forum | Sun Sep 12 12:45:56 EDT 2010 | tony1
Hi there, does anyone experience in NiPdAu solderability dip & look test? I experiencing solder non wet issue on side I/O & also center ground for QFN package. Appreciate someone can offer me a solution. Thanks
Electronics Forum | Fri Sep 19 15:23:33 EDT 2008 | vladig
All I can say is my regular "Get it analyzed", so you'll know what the streak is. Regards, Vladimir
Electronics Forum | Sat Sep 20 09:31:42 EDT 2008 | vladig
Wise move :-) Please let me know the results of the analysis and we can take it from there. Vlad
Electronics Forum | Thu Sep 18 23:56:56 EDT 2008 | trynders
am having wetting issues with two Burr Brown Op amps. Both are SOICs with NiPdAu lead frame finishes. I have attached a photo that shows a black streak the length of the lead (before soldering). This appearance is consistent of all leads and is exist
Electronics Forum | Fri Sep 19 15:52:18 EDT 2008 | davef
This is not something that we'd expect to see on NiPdAu finished leads. Help us understand the extent of the problem better. From your picture, it looks like a band of copper color with black on the outer portions of the copper color that bleeds int
Electronics Forum | Tue Apr 26 03:28:26 EDT 2005 | Just mee
What test is applicable to check for QFN package with NiPdAu leadframe if leads/pad are solderable? what are the options other than dip and look solderability testing? Thanks,
Electronics Forum | Fri Sep 19 21:31:15 EDT 2008 | trynders
Thanks for the response guys! The parts are being sent to a local lab as we speak. I'll let you know the results when I get them. I am not sure the purpose of the copper band, but the black around the band is just shadowing from how I took the pi
Electronics Forum | Mon Apr 16 09:12:23 EDT 2007 | davef
Standard for appearance: J-STD-001 and IPC-A-610 committees eliminated the requirement that solder connections be "bright and shiny". Certain solderability protections; such as Au, NiPd, NiPdAu; can affect the surface texture of a solder connection,