Electronics Forum | Sat Sep 12 09:49:38 EDT 2015 | davef
If the boards were still "wet" after DI wash, your [I assume] low res flux could be reacting with the moisture on the board and causing the white spots. The preheater in the wave could have more dryification than the preheater on the selective solde
Electronics Forum | Fri Sep 11 15:27:50 EDT 2015 | u4bga
Hi! We're noticing white spots on 2 PCBAs after the selective soldering & DI Wash processes. ----Facts---- 1) The marking is on all boards, irrespective of date code 2) It only happens on leads that have been selective soldered 3) The pattern of w
Electronics Forum | Mon Nov 30 23:45:20 EST 1998 | Kallol Chakraborty
Hi folks , Lately we are seeing a lot of rawcards with black spots on the pads - most of them have Au finish(immersion gold) . We did a lot of inspecton after wave solder and found that only (fine pitch) QFP are affected the most. Our inspection /te
Electronics Forum | Tue Dec 01 07:24:44 EST 1998 | Earl Moon
| Hi folks , | Lately we are seeing a lot of rawcards with black spots on the pads - most of them have Au finish(immersion gold) . We did a lot of inspecton after wave solder and found that only (fine pitch) QFP are affected the most. Our inspection
Electronics Forum | Tue Dec 01 07:54:49 EST 1998 | kallol chakraborty
| | Hi folks , | | Lately we are seeing a lot of rawcards with black spots on the pads - most of them have Au finish(immersion gold) . We did a lot of inspecton after wave solder and found that only (fine pitch) QFP are affected the most. Our inspec
Electronics Forum | Sun May 13 21:02:34 EDT 2001 | djarvis
Gary, You're not trying to clean these boards with Iso or other solvents after using no-clean solder paste? That'll do it.
Electronics Forum | Tue Dec 01 09:02:18 EST 1998 | Earl Moon
| | | Hi folks , | | | Lately we are seeing a lot of rawcards with black spots on the pads - most of them have Au finish(immersion gold) . We did a lot of inspecton after wave solder and found that only (fine pitch) QFP are affected the most. Our in
Electronics Forum | Fri Dec 04 20:26:34 EST 1998 | kallol Chakraborty
| | | | Hi folks , | | | | Lately we are seeing a lot of rawcards with black spots on the pads - most of them have Au finish(immersion gold) . We did a lot of inspecton after wave solder and found that only (fine pitch) QFP are affected the most. Ou
Electronics Forum | Fri Dec 04 20:37:45 EST 1998 | kallol chakraborty
| | | | | Hi folks , | | | | | Lately we are seeing a lot of rawcards with black spots on the pads - most of them have Au finish(immersion gold) . We did a lot of inspecton after wave solder and found that only (fine pitch) QFP are affected the most
Electronics Forum | Fri May 11 15:43:41 EDT 2001 | davef
More information would be helpful. For instance: * Talk about the distribution of the problem, including a single lot or from various lots and over components and component types on the board * Tell us about the board (ie, thickness, type, solder ma