Printed Circuit Board Assembly & PCB Design Forum
SMT electronics assembly manufacturing forum.
Views: 6143
Hello to all,
I am using ersa versaflow 3 selective solde...
- Feb 08, 2017
by
Mile
what kind of contamination are you dealing with?
ultrason...
- Feb 09, 2017
by
bukas
Thanks for your answer, contamination in form of fine dust p...
- Feb 09, 2017
by
Mile
is it yellow dust? if yes,
1. you will probably need to cl...
- Feb 10, 2017
by
bukas
I've been using the ERSA Versaflow 3/45 for 3 years. I've be...
- Feb 10, 2017
by
LSI ADL
Contamination color is silver dust, like ash dust from burni...
- Feb 10, 2017
by
Mile
I would email Chad at ERSA and see what he might have to say...
- Feb 13, 2017
by
LSI ADL
I am posting some pictures of the conteiment, i am using lea...
- Feb 14, 2017
by
Mile
yep, thats it. you will need to clean the whole pot. I used ...
- Feb 15, 2017
by
bukas
The main problem is that we changed the whole pot 1 year ago...
- Feb 15, 2017
by
Mile
My company has had the same issue on our Versaflow 366 with ...
- Mar 11, 2017
by
Tim
I had a nitrogen salesman in yesterday. He brought his tech...
- Mar 14, 2017
by
Stephen