0603 component drift

#8576

0603 component drift | 11 November, 1999

We are having a continuing problem with 0603 chip capacitors not centering themselves on the pads during the reflow process, causing an open condition at one end. Does anyone know what can be done to alleviate this? Thanks much.

Gary

reply »

#8577

Re: 0603 component drift | 11 November, 1999

Gary: Sounds like the spacing between each pad for the component are too far apart. My 2�. Dave F

reply »

Leland Woodall

#8578

Re: 0603 component drift | 20 June, 2000

Gary,

We've experienced the same problem in the past, and found that moving the stencil apertures closer together solved the dilemma. This was a much easier solution than having to redesign the PWB.

Leland