Electronics Forum | Tue Sep 16 17:03:34 EDT 2014 | rangarajd
We have an issue with solder wicking up the leads/ inside terminations on an SMT connector. The solder coverage is sometimes over 50% of the connectors inside pin length. The terminations are gold plated. Is there an IPC spec for acceptability? Plea
Electronics Forum | Sun Sep 21 10:03:15 EDT 2014 | gascon5383
hi, there is an IPC standard, IPC-A-610 - Acceptability of Electronic Assemblies. According to this manual, solder in the bends of a lead does not matter, but solder touching the body of a component is a defect. I cannot find a specific reference in
Electronics Forum | Sun Aug 23 20:24:59 EDT 1998 | Karlin
Hi, Does anyone has experiences in reflowing Ceramic BGA and found solder wicking ? Solder wicking has the syndrome that solder being wick from the pad and ended up in the leads. We have rule out the possibility of not printing any solder paste there
Electronics Forum | Mon Oct 22 10:51:48 EDT 2007 | davef
You say, "we have encountered solder wicking on components ..." We expect to see wicking on solder connections. Maybe we're just using different terminology. Please describe the problem that you're seeing.
Electronics Forum | Thu Jul 17 04:42:47 EDT 2003 | sanjeevc
Hi! One technique: 1. Remove all balls 2.Make > a mask(stensil)for reballing.The holes of the > mask must be 0.8-0.9 the size of the pads. 3. > Reball chips 4. Reflow chips Good luck Hi Yes,we have done quite a bit of reballing of BGAs with
Electronics Forum | Mon Aug 24 08:34:14 EDT 1998 | JUSTIN MEDERNACH
| Hi, | Does anyone has experiences in reflowing Ceramic BGA and found solder wicking ? Solder wicking has the syndrome that solder being wick from the pad and ended up in the leads. | We have rule out the possibility of not printing any solder paste
Electronics Forum | Tue Oct 23 03:57:39 EDT 2007 | jkhiew
Thanks Dave. But I do not understand why the solder being wicking away by the component itself. Does Ag/Pd finishes has stronger wettability than LF HASL finishes ? Rgds
Electronics Forum | Mon Oct 22 05:04:08 EDT 2007 | jkhiew
Hi, Recently we have encountered solder wicking on components termination (total of 13 pcs of components on one pcb)with Ag/Pd finishes during lead-free reflow soldering. The pcb is LF HASL surface finish and LF solder paste composition is SAC305.We
Electronics Forum | Mon Aug 24 21:04:58 EDT 1998 | Karlin
| | Hi, | | Does anyone has experiences in reflowing Ceramic BGA and found solder wicking ? Solder wicking has the syndrome that solder being wick from the pad and ended up in the leads. | | We have rule out the possibility of not printing any solder
Electronics Forum | Tue Oct 23 07:03:52 EDT 2007 | davef
We're not really sure. Usually when solder leaves the pads and wicks-up a component lead, it means the component lead is much warmer than the pad on the board. This is the direction we would have taken this if we hadn't taken the AgPd / conductive e